Producent dzianin od 2009 · Chiny

METODA BADAWCZA · ISO 105-E04

Odporność wybarwienia na pot ISO 105-E04

ISO 105-E04 określa, czy tkanina zmienia barwę lub plami inne tkaniny w sztucznym pocie, badane w roztworze alkalicznym i kwasowym. Amerykańskim odpowiednikiem jest AATCC 15.

Próbki pobrane z partii produkcyjnej.
 – Szczegóły dzianiny z katalogu Runtang
Norma

ISO 105-E04

Odpowiednik amerykański

AATCC 15

Roztwory

Alkaliczny pH 8,0 · kwasowy pH 5,5

Ocena

Skale szare, 1–5

01

What This Test Measures

A fabric and multifibre composite is soaked in artificial perspiration made with L-histidine, held under pressure at body temperature, dried and graded for colour change and staining. It matters most for T-shirts, sportswear and underwear.

02

How We Run It in Our Lab

Our technicians follow a written work instruction for this method.

Alkaline and acid tests run in parallel on separate specimens.

01

Prepare Solutions

Alkaline solution at pH 8.0 and acid solution at pH 5.5, both with L-histidine and sodium chloride.

02

Soak

Each 40 × 100 mm composite is soaked at a liquor ratio of 50:1 for 30 minutes, then excess solution is removed.

03

Hold Under Pressure

Specimens are held between resin plates under 12.5 kPa at 37 ± 2 °C for 4 hours.

04

Dry and Grade

Dried at no more than 60 °C. Graded with the ISO 105-A02 grey scale for colour change and A03 for staining (AATCC EP1/EP2 for AATCC methods), under the agreed light source in a light booth, by at least two technicians.

03

Test Conditions

Key settings. Write the method and procedure in your specification.

ParameterSetting
RoztworyAlkaline pH 8.0 and acid pH 5.5 (AATCC 15: one acid solution)
Liquor ratio50:1, 30 minutes at room temperature
Pressure and incubation12.5 kPa; 37 ± 2 °C for 4 hours
OcenaSkale szare, 1–5
Equivalent methodsAATCC 15 (US) · GB/T 3922 (China). Compare methods →
04

Results for Your Order

Ask us for results for the selected fabric, shade and test conditions. Acceptance values for your order are agreed in writing.

05

Writing This Test into Your Specification

Ask for Both Solutions

Specify alkaline and acid results; one fabric can behave differently in each.

Separate Change and Staining

Give one grade for colour change and one for staining.

Think About End Use

For sportswear and underwear, perspiration fastness matters as much as washing fastness.

06

Questions About ISO 105-E04

Why are there two perspiration solutions in ISO 105-E04?

Sweat can be mildly alkaline or acid. ISO 105-E04 tests both, at pH 8.0 and pH 5.5. AATCC 15 uses one acid solution.

How long is the perspiration test?

Soaking takes 30 minutes, then 4 hours at 37 °C under 12.5 kPa, followed by drying and grading.

Which garments need perspiration fastness?

Garments worn close to the skin or during exercise: T-shirts, sportswear, underwear and nightwear.