2009년부터 이어온 니트 원단 제조사 · 중국

시험 방법 · ISO 12945-1

필링 저항성 ISO 12945-1

ISO 12945-1은 코르크로 안감을 댄 박스에서 회전시킨 후의 필링을 측정합니다. 일반 면 니트는 3등급 이상으로 측정되며, 4등급은 매우 우수한 결과입니다. 미국 규격에서는 흔히 ASTM D3512를 대신 사용합니다.

대량 로트에서 시편을 채취합니다.
 – Runtang 카탈로그의 원단 상세 정보
표준

ISO 12945-1:2020 (박스)

미국 시험 방법

ASTM D3512 / D4970

면 니트

3등급 이상; 4등급 매우 우수

등급 판정

1–5

01

What This Test Measures

Specimens on tubes are tumbled in a cork-lined box for an agreed number of revolutions, then compared with reference photographs in a viewing cabinet and graded from 5 (no pilling) to 1 (very severe).

The revolutions decide how hard the test is. Specifications we receive range from 7,200 to 14,400 revolutions, so a grade needs its revolutions next to it.

02

How We Run It in Our Lab

Our technicians follow a written work instruction for this method.

01

Cut and Mount

Specimens in length and width are sewn into tubes and mounted.

02

Tumble

Tubes tumble in the cork-lined box for the agreed revolutions.

03

Assess

Specimens are compared with reference photographs in a viewing cabinet.

04

Grade

Each specimen is graded 1–5 by at least two technicians.

03

Test Conditions

Key settings. Write the method and procedure in your specification.

ParameterSetting
ApparatusPilling box with cork lining
RevolutionsAs agreed, e.g. 7,200, 10,800 or 14,400
EvaluationViewing cabinet with oblique light
등급 평가5 = no pilling, 1 = very severe
Equivalent methodsASTM D3512 / D4970 (US) · GB/T 4802.3 (China). Compare methods →
04

Measured Range and Buyer Values

Results depend on fibre, construction, shade and finishing.

Fabric / shade당사 측정 범위Values in buyer specifications
Regular 100% cotton knitsGrade 3 and above; 4 is very goodGrade 4 at 14,400 rev; 4-5 at 10,800 rev

“Our measured range” comes from our own test records on bulk lots. “Values in buyer specifications” are requirements we have received; the value that applies to your order is the one written into it. — Xiwen Zhang, Co-founder & CEO

05

Writing This Test into Your Specification

State the Revolutions

Write the grade with its revolutions, for example “grade 3-4 after 7,200 revolutions”.

Name the Instrument

Pilling box, random tumble (ASTM D3512) and Martindale give different grades.

Ask About Options

Combed or compact yarns, enzyme bio-polishing and anti-pilling finishes can raise the grade. Ask before production.

06

Questions About ISO 12945-1

What pilling grade is good for a cotton knit?

For regular 100% cotton knits, grade 3 and above in ISO 12945-1 is generally acceptable and grade 4 is a very good result.

Why does the number of revolutions matter?

More revolutions mean more abrasion; the same fabric can be grade 4 after 7,200 revolutions and grade 3 after 14,400.

Is ISO 12945-1 the same as ASTM D3512?